Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® A3K FC Aqua UN - PA66 - BASF

Material Data Center offers the following functions for Ultramid® A3K FC Aqua UN:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultramid A datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明
Ultramid® A3K FC Aqua UN is optimized for plastic parts, mandatory requiring material approvals for drinking water or direct food contact.

The product is approved according to
• 21 CFR FDA § 177.1500 "Nylon resins" (except contact with alcoholic beverages)
• European Food Contact European Food Contact Commission Regulation (EU) 10/2011
• GMP (EC) n°2023/2006

and provides the approvals for drinking water regulations of
• KTW
• DVGW W270
• WRAS
• ACS (disclosure of ingredients)
• NSF (disclosure of ingredients)

For questions regarding the compliance with further regulations, and certificates, please contact your local BASF representative or Plastics Safety (E-Mail: plastics.safety@basf.com).
加工/物理特性干 / 已调节单位Test Standard
ISO数据
熔体体积流动速度, MVR 115 / * cm³/10min ISO 1133
温度 275 / * °C -
载荷 5 / * kg -
模塑收缩率, 平行 1.6 / * % ISO 294-4, 2577
模塑收缩率, 垂直 1.8 / * % ISO 294-4, 2577
喷射温度 180 °C -
机械性能干 / 已调节单位Test Standard
ISO数据
拉伸模量 3100 / 1100 MPa ISO 527
屈服应力 85 / 50 MPa ISO 527
屈服伸长率 5 / 20 % ISO 527
名义断裂伸长率 30 / >50 % ISO 527
弯曲模量, 23°C 2900 / - MPa ISO 178
拉伸蠕变模量, 1h * / 1100 MPa ISO 899-1
拉伸蠕变模量, 1000h * / 700 MPa ISO 899-1
无缺口简支梁冲击强度, +23°C N / N kJ/m² ISO 179/1eU
简支梁冲击强度, -30°C N / - kJ/m² ISO 179/1eU
简支梁缺口冲击强度, +23°C 5 / 20 kJ/m² ISO 179/1eA
简支梁缺口冲击强度, -30°C 4 / - kJ/m² ISO 179/1eA
悬臂梁缺口冲击强度, +23°C 5.5 / N kJ/m² ISO 180/1A
悬臂梁缺口冲击强度 6 / - kJ/m² ISO 180/1A
悬臂梁缺口冲击强度 - 温度 -30 °C -
热性能干 / 已调节单位Test Standard
ISO数据
熔融温度, 10°C/min 260 / * °C ISO 11357-1/-3
玻璃化转变温度, 10°C/min 72 / * °C ISO 11357-1/-2
热变形温度, 1.80 MPa 75 / * °C ISO 75-1/-2
热变形温度, 0.45 MPa 220 / * °C ISO 75-1/-2
维卡软化温度, B 250 / * °C ISO 306
线性热膨胀系数, 平行 98 / * E-6/K ISO 11359-1/-2
1.5mm名义厚度时的燃烧性 V-2 / * class IEC 60695-11-10
测试用试样的厚度 1.6 / * mm -
燃烧性-氧指数 28 / * % ISO 4589-1/-2
电性能干 / 已调节单位Test Standard
ISO数据
相对介电常数., 100Hz 3.8 / - - IEC 62631-2-1
相对介电常数., 1MHz 3.2 / 5 - IEC 62631-2-1
介质损耗因子, 100Hz 50 / - E-4 IEC 62631-2-1
介质损耗因子, 1MHz 250 / 2000 E-4 IEC 62631-2-1
体积电阻率 1E13 / 1E10 Ohm*m IEC 62631-3-1
表面电阻率 * / 1E10 Ohm IEC 62631-3-2
相对漏电起痕指数 - / 600 - IEC 60112
其它性能干 / 已调节单位Test Standard
吸水性 8.5 / * % 类似ISO 62
吸湿性 2.8 / * % 类似ISO 62
密度 1130 / - kg/m³ ISO 1183
Bulk density 700 kg/m³ -
模塑测量的特殊性能干 / 已调节单位Test Standard
ISO数据
粘数 150 / * cm³/g ISO 307, 1157, 1628
试样制备条件价值单位Test Standard
ISO数据
注塑, 熔体温度 290 °C ISO 294
注塑, 模具温度 80 °C ISO 294
注塑, 注射速度 200 mm/s ISO 294
加工推荐(注塑)价值单位Test Standard
预干燥-温度 80 °C -
预干燥-时间 4 h -
加工湿度 ≤0.15 % -
注塑熔体温度 280 - 300 °C -
模具温度 60 - 80 °C -
函数
粘度-剪切速度 , Ultramid® A3K FC Aqua UN, PA66, BASF
剪切应力-剪切速度 , Ultramid® A3K FC Aqua UN, PA66, BASF
动态剪切模量-温度 , Ultramid® A3K FC Aqua UN (烘干), PA66, BASF
动态剪切模量-温度 , Ultramid® A3K FC Aqua UN (状况), PA66, BASF
应力-应变.  , Ultramid® A3K FC Aqua UN (烘干), PA66, BASF
应力-应变.  , Ultramid® A3K FC Aqua UN (状况), PA66, BASF
正割模量-应变.  , Ultramid® A3K FC Aqua UN (烘干), PA66, BASF
正割模量-应变.  , Ultramid® A3K FC Aqua UN (状况), PA66, BASF
应力-应变(等时的) 23°C, Ultramid® A3K FC Aqua UN (状况), PA66, BASF
蠕变模量-时间. 23°C, Ultramid® A3K FC Aqua UN (状况), PA66, BASF
蠕变曲线 23°C, Ultramid® A3K FC Aqua UN (状况), PA66, BASF
应力-应变(等时的) 60°C, Ultramid® A3K FC Aqua UN (烘干), PA66, BASF
蠕变模量-时间. 60°C, Ultramid® A3K FC Aqua UN (烘干), PA66, BASF
蠕变曲线 60°C, Ultramid® A3K FC Aqua UN (烘干), PA66, BASF
应力-应变(等时的) 90°C, Ultramid® A3K FC Aqua UN (烘干), PA66, BASF
蠕变模量-时间. 90°C, Ultramid® A3K FC Aqua UN (烘干), PA66, BASF
蠕变曲线 90°C, Ultramid® A3K FC Aqua UN (烘干), PA66, BASF
应力-应变(等时的) 120°C, Ultramid® A3K FC Aqua UN (烘干), PA66, BASF
蠕变模量-时间. 120°C, Ultramid® A3K FC Aqua UN (烘干), PA66, BASF
蠕变曲线 120°C, Ultramid® A3K FC Aqua UN (烘干), PA66, BASF
比容-温度(pvT) , Ultramid® A3K FC Aqua UN, PA66, BASF
拉伸模量-温度 , Ultramid® A3K FC Aqua UN (烘干), PA66, BASF
拉伸模量-温度 , Ultramid® A3K FC Aqua UN (状况), PA66, BASF
典型数据
加工方法
注塑, 其它挤出成型
供货形式
粒料, 自然色
添加剂
润滑剂, 脱模助剂
特殊性能
经热稳处理的/耐热的
Certifications
可食品接触的, 10/2011认证, FDA 21 CFR认证, 可水接触的, 可水接触的(KTW), 可水接触的(DVGW W270), NSF认证 61
应用
汽车
地区供应
其他信息
注塑成型
PREPROCESSING
Pre/Post-processing, max. allowed water content: .15 %
Pre/Post-processing, Pre-drying, Temperature: 80 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 280 - 300 °C
injection molding, Melt temperature, recommended: 290 °C
injection molding, Mold temperature, range: 60 - 80 °C
injection molding, Mold temperature, recommended: 60 °C
injection molding, Dwell time, thermoplastics: 10 min
耐化学性
酸类
醋酸 (5g/100g) (23°C)
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.